Higher Tensile Steel in Hull Design
Higher tensile steel in hull design: AH32, AH36 and DH36 grades, the UR S4 material factor k, YP47, steel grade classes, and the fatigue and buckling limits.
Contents17 sections
Higher tensile steel is hull structural steel with a minimum yield stress above the 235 N/mm² of normal strength steel. It reduces the required scantlings where the hull girder stress is highest. IACS UR W11 Rev.9 (May 2017) covers three higher strength levels: 315, 355 and 390 N/mm². IACS UR S4 Rev.4 (April 2017) sets the material factor k that the strength rules apply to them.
AH36, the most named grade, is steel of 355 N/mm² minimum yield, impact tested at 0 °C, with k = 0.72. Higher tensile steel lowers the required section modulus and the plate thickness. It does not raise the stiffness, the minimum thicknesses or the corrosion addition, and it does not raise the fatigue strength of a welded joint. The hull strength and longitudinal bending article covers the checks that use k.
Steel grades and their designations
A hull steel grade names two properties: the strength level and the toughness, given by the Charpy impact test temperature. IACS UR W11 Rev.9 1.3 describes “three strength levels (315, 355 and 390 N/mm2) each subdivided into four grades”, plus the normal strength grades A, B, D and E. The CSR writes the higher strength grades as AH32, AH36 and AH40. UR W11 writes them as A32, A36 and A40.
Figure 1 shows the grades by strength level and test temperature.
Charpy V-notch impact test temperature
Values from IACS UR W11 Rev.9 (May 2017) and UR W31 Rev.3 (March 2023).
Strength and toughness values
UR W11 Rev.9 Tables 6 and 7, and CSR Pt 1 Ch 3 Sec 1 Table 1, give these values:
| Strength level | Minimum yield ReH (N/mm²) | Tensile strength Rm (N/mm²) | Elongation A5 | Charpy energy, t ≤ 50 mm, long./trans. |
|---|---|---|---|---|
| Normal strength, A to E | 235 | 400 to 520 | 22% | 27/20 J (grade A: not required to 50 mm) |
| 32 | 315 | 440 to 570 | 22% | 31/22 J |
| 36 | 355 | 490 to 630 | 21% | 34/24 J |
| 40 | 390 | 510 to 660 | 20% | 39/26 J |
The test temperatures follow the letter. Normal strength grades A, B, D and E are tested at +20, 0, −20 and −40 °C. Higher strength grades A, D, E and F are tested at 0, −20, −40 and −60 °C. Grade B normal strength steel is “generally not required” to have a Charpy test up to 25 mm.
UR W11 covers plates and wide flats up to 100 mm, and sections and bars up to 50 mm (1.2). The CSR Table 1 values apply to an as-built thickness of 100 mm or less. CSR Pt 1 Ch 3 Sec 1 [2.1.2] calls 235 N/mm² steel “normal strength hull structural steel”, labelled MS. The higher strengths are labelled HT. [2.1.1] takes E as 206,000 N/mm² and Poisson’s ratio as 0.3 for all carbon steel.
Thicker plates and special steels in UR W11
The Charpy energy rises with thickness for normal strength steel. Grade A needs no Charpy test up to 50 mm (Table 6). From 50 to 70 mm it needs 34/24 J, and from 70 to 100 mm 41/27 J. Note (5) to Table 6 allows an exemption for grade A over 50 mm in fine grain normalized steel. The yield stress is measured as ReH, or as the proof stress Rp0.2 where no yield point shows (6.1).
The impact values apply to standard 10 × 10 mm specimens (6.3). Below 10 mm thickness the test can be waived, at the discretion of the classification society, or made on sub-size specimens under UR W2. UR W11 1.4 places other steels under “special approval” with a special designation. Clause 1.5 covers the corrosion resistant steels for cargo oil tanks, up to 50 mm. SOLAS regulation II-1/3-11 allows them under MSC.289(87); Rev.10 moves the clause to 1.6.
The revisions of UR W11 apply by contract date. Rev.8 applied to ships contracted on or after 1 July 2015 and Rev.9 to those on or after 1 July 2018. The Charpy V-notch impact test at the grade temperature proves the toughness, apart from the exemptions stated above.
What changes in UR W11 Rev.10
IACS UR W11 Rev.10 (September 2025) applies to ships contracted for construction on or after 1 January 2027. It also applies to steel product certification or manufacturer approval applications from that date. The strength levels and the tensile values are unchanged. Clause 1.5 covers high heat input welding over 50 kJ/cm, “where manufacturers optionally select approval”. Rev.9 already covered that welding in its Appendix B.
UR W16 is not a hull steel rule
IACS UR W16 Rev.3 (March 2016), “High Strength Steels for Welded Structures”, covers steels of 420 to 960 N/mm². Clause 1.1 states that UR W16 does “not apply to steels intended for hull structure of commercial ships whose requirements are specified in Unified Requirement W11”. Rev.4 applies from 1 January 2027. The YP47 hull steel of container ships is in UR W31, not W16.
The material factor k and UR S4
IACS UR S4 Rev.4 (April 2017) defines the material factor k for higher tensile steel, and nothing else. Its title is “Criteria for the Use of High Tensile Steel with Minimum Yield Stress of 315 N/mm2, 355 N/mm2 and 390 N/mm2”. The UR is one page. It states: “This UR does not apply to CSR Bulk Carriers and Oil Tankers.”
Material factor k
where
| \(k\) | material factor for higher tensile steel; 1.0 for mild steel under UR S7 and the CSR | |
| \(0.66\) | for 390 N/mm² steel, provided that a fatigue assessment to the Society's requirements is performed | |
| \(0.68\) | for 390 N/mm² steel in other cases | |
| \(R_{eH}\) | specified minimum yield stress | N/mm² |
UR S4 gives no value for mild steel. UR S7.1 gives “k = 1.0 for ordinary hull structural steel, k < 1.0 for higher tensile steel according to S4”. UR S4 also sets no rule on how far higher tensile steel extends, and no buckling condition. Those are in the UR S11 and CSR checks.
The history of UR S4 runs from 1973 through Rev.1 (1974), Rev.2 (April 2007) and Rev.3 (May 2010) to Rev.4 (April 2017).
The two values for 390 N/mm² steel
UR S4 gives k = 0.66 for 390 N/mm² steel “provided that a fatigue assessment of the structure is performed to verify compliance with the requirements of the Society”. UR S4 gives 0.68 “in other cases”. UR S4 does not define the fatigue assessment, so each society’s method governs. The fatigue assessment of ship structures article covers those methods.
The CSR material factor
CSR Pt 1 Ch 3 Sec 1 [2.2.1] Table 2 gives k of 1.00, 0.78, 0.72 and 0.68 at 235, 315, 355 and 390 N/mm². “For intermediate values of ReH, k is obtained by linear interpolation.” Steel above 390 N/mm² is “considered by the Society on a case-by-case basis”. The CSR has no 0.66 option and no entry for 460 N/mm².
CSR [2.1.4] covers ReH other than 235 N/mm²: “hull girder strength and hull scantlings are to be determined by taking into account the material factor, k”. The IACS Common Structural Rules therefore apply k in both the hull girder and the local checks.
How the material factor k enters the hull girder checks
The material factor divides the permissible hull girder stress, so a lower k allows a higher stress and a smaller section modulus. UR S11.3.1.1 sets a permissible bending stress of 175/k N/mm² for non-CSR ships, and S11.4 a permissible shear stress of 110/k N/mm². The required section modulus is therefore proportional to k.
The CSR uses the same principle with its own values.
Permissible hull girder bending stress at sea
where
| \(\sigma_{perm}\) | permissible stress, seagoing static plus dynamic, in the midship region | N/mm² |
| \(k\) | material factor, CSR Pt 1 Ch 3 Sec 1 Table 2 | |
| \(\sigma_{perm,ends}\) | permissible stress towards the ends; harbor values 143/k and 105/k | N/mm² |
For AH36 steel, 190/k gives 263.9 N/mm² in the midship region at sea, against 190 N/mm² for mild steel. UR S11A for container ships uses 235/(1.24 k), which the UR S11A article covers.
What k does not change
The minimum stiffness of the hull girder does not fall with higher tensile steel. CSR Pt 1 Ch 5 Sec 1 [2.3.1] sets IyR = 2.7 Cw L³ B (CB + 0.7) × 10⁻⁸ m⁴, with no k. UR S11.3.1.2 sets the minimum amidships at 3 C L³ B (Cb + 0.7) cm⁴, also with no k. The CSR minimum section modulus, ZR = 0.9 k Cw L² B (CB + 0.7) × 10⁻⁶ m³, does carry k.
Figure 2 shows how the required section modulus, the plate thickness and the moment of inertia change with the yield stress.
Where k enters the CSR checks
CSR [2.1.4] applies k to the hull scantlings as well as the hull girder. The yielding check compares the permissible stress, divided by k, with the stress from the still water bending moment. The stress from the rule wave bending moment adds to it. The CSR also gives harbor permissible values of 143/k in the midship region and 105/k at the ends.
For aluminum, CSR [4.4.1] takes k = 235/R’lim, with R’lim the limit stress of the alloy. The same factor structure therefore covers a material other than steel.
Worked example: deck modulus with AH36
Take a non-CSR ship whose UR S11 required section modulus in mild steel is 20.0 m³ at the deck. These are example values.
- Find k for AH36. UR S4 gives 0.72.
- Find the required modulus. 20.0 × 0.72 = 14.4 m³.
- Find the permissible stress. 175/0.72 = 243.1 N/mm².
- Check the stiffness. The UR S11.3.1.2 minimum moment of inertia is unchanged, so it can govern once the modulus falls.
The deck saves 28% of its required modulus. The hull girder deflects more for the same moment, because E and the inertia limit are unchanged.
Worked example: when the inertia minimum governs
Take a ship with L of 200 m, B of 32.26 m and Cb of 0.82. These are example values.
- Find the wave coefficient. UR S11 gives C = 10.75 − ((300 − 200)/100)^1.5 = 9.75.
- Find the minimum inertia. 3 × 9.75 × 200³ × 32.26 × 1.52 = 1.147 × 10¹⁰ cm⁴, or 114.7 m⁴.
- Compare with the modulus. With the deck 11.0 m above the neutral axis, 14.4 m³ needs about 158 m⁴.
- Decide. 158 m⁴ exceeds 114.7 m⁴, so the modulus still governs in this example.
With a lower k, or a neutral axis closer to the deck, the inertia minimum can govern instead. The steel saved by higher tensile steel then stops at the stiffness limit.
How yield stress enters the local scantlings
For plating under lateral pressure, the required thickness falls roughly with the square root of the yield stress, not in proportion to it. CSR Pt 1 Ch 6 Sec 4 [1.1.1] gives the net plate thickness as t = 0.0158 αp b √(|P|/(χ Ca ReH)). For “other members”, Ca is a fixed 0.8, so t is proportional to 1/√ReH.
For AH36, √(235/355) = 0.814, so the plating is about 81% of the mild steel thickness. For longitudinal members, Ca depends on the hull girder stress σhg/ReH, so the ratio is not a simple square root. These ratios are Shipping-Wiki.com arithmetic from the CSR formula.
Worked example: plating thickness with AH36
Take an “other member” plate of 15.0 mm net thickness in mild steel under lateral pressure, with a corrosion addition of 2.5 mm. These are example values.
- Find the thickness ratio for AH36. √(235/355) = 0.814.
- Find the net thickness in AH36. 15.0 × 0.814 = 12.2 mm.
- Add the corrosion addition. The gross plate is 14.7 mm in AH36 against 17.5 mm in mild steel.
- Find the share of the addition: 17% of the AH36 gross plate and 14% of the mild steel one.
The steel saving is 16% of the gross thickness here, less than the 19% of the net thickness. The unchanged corrosion addition takes up part of the saving.
Minimum thickness and corrosion addition
CSR Pt 1 Ch 1 Sec 2 [5.2.1] describes the minimum thickness as “independent of the specified minimum yield stress”. A thin member at its minimum thickness gains nothing from higher tensile steel. CSR Pt 1 Ch 3 Sec 3 [1.1.1] applies the corrosion additions “to carbon-manganese steels” with no distinction by strength.
The corrosion addition is therefore the same absolute thickness on thinner higher tensile plating. It is a larger share of the plate. The hull thickness measurement at survey compares the gauged plate with the renewal criteria of its as-built thickness.
What higher tensile steel does not improve
Higher tensile steel raises the yield-based limits only. Stiffness, elastic buckling and welded fatigue strength stay as they are for mild steel.
Buckling
The elastic buckling stress of a plate depends on E and the plate slenderness, σE = π² E/(12(1 − ν²)) (tp/b)², with no yield term. A thinner higher tensile plate has a lower elastic buckling stress than the mild steel plate it replaces.
The yield enters the critical stress only where the elastic buckling stress exceeds half the yield, through the Johnson-Ostenfeld correction of UR S11.5.3.1. The buckling of ship plating and stiffeners article covers the check. CSR Pt 1 Ch 8 Sec 2 [2.1.1] sets a slenderness limit tp ≥ (b/C) √(ReH/235). Higher tensile plating therefore needs a thicker plate for the same spacing.
Fatigue
IACS UR W11 Rev.9 2.3 Note 1 states: “when fatigue loading is present, the effective fatigue strength of a welded joint of higher strength steel may not be greater than that of a welded joint in normal strength steels.” The welded joint S-N curves of CSR Pt 1 Ch 9 Sec 3 do not depend on the yield stress. A thinner plate at a higher stress therefore has a shorter fatigue life.
The CSR fatigue check applies to steels up to 390 N/mm² (Pt 1 Ch 9 Sec 1 [1.1.5]). The yield stress enters the CSR fatigue check in two narrow places. Free plate edges take a material factor fmaterial = 1200/(965 + ReH) (Ch 9 Sec 3 [3.1.3]). The mean stress correction uses ReEq = max(315, ReH) (Ch 9 Sec 3 [3.2.1]). The 0.66 value of k for 390 N/mm² steel in UR S4 is conditional on a fatigue assessment.
Stiffness and deflection
E is 206,000 N/mm² for all carbon steel grades (CSR [2.1.1]). A hull built with less steel deflects more under the same load. The minimum moment of inertia, without k, limits that deflection for the hull girder.
Ultimate strength and whipping
The yield stress enters the hull girder ultimate strength through the load-end shortening curves of CSR Pt 1 Ch 5 App 2. Their plate slenderness βE rises with ReH and with a thinner plate, so a thinner higher tensile deck has a smaller effective width. The whipping check of large container ships uses the same capacity.
Owner’s limit on higher tensile steel
CSR Pt 1 Ch 1 Sec 2 [3.10.1] lists among the owner’s extras a “Maximum percentage of high strength steel”. An owner can therefore cap the use of higher tensile steel in the building contract, above the rule minimums.
Where higher tensile steel goes: extent rules
Higher strength steel in the deck or the bottom extends towards the neutral axis until the steel beyond it is within its own limit. CSR Pt 1 Ch 5 Sec 1 [2.4.1] sets the vertical extent.
Vertical extent of higher strength steel
where
| \(z_{hts,i}\) | vertical extent of the higher strength steel from the deck or the bottom | m |
| \(z_{1}\) | distance from the neutral axis to the deck or the bottom | m |
| \(\sigma_{L}\) | hull girder bending stress at the deck or the bottom | N/mm² |
| \(\sigma_{perm,i}\) | permissible hull girder stress of the considered steel | N/mm² |
CSR [2.4.2] continues the higher strength steel along the length until the stress falls within the allowable value of mild steel. The strength deck and the bottom, the flanges of the hull girder, are therefore where higher tensile steel goes first. The bottom shell of the double bottom and the deck plating lie farthest from the neutral axis, where the bending stress is highest.
Worked example: the vertical extent
Take a section with the deck 10 m above the neutral axis and a hull girder stress σL of 250 N/mm² at the deck. The steel below the higher strength band is mild steel with σperm of 190 N/mm². These are example values.
- Find the stress ratio. 190/250 = 0.76.
- Find the extent. 10 × (1 − 0.76) = 2.4 m.
- Apply it. The higher strength steel extends at least 2.4 m down from the deck.
The stress falls linearly towards the neutral axis. At 2.4 m below the deck it is 0.76 × 250 = 190 N/mm², the permissible value of the mild steel.
Steel grades by member: UR S6
IACS UR S6 Rev.9 Corr.2 (November 2021) sets the steel grade of each hull member from its material class and its as-built thickness. UR S6 applies to ships of 90 m in length and above, from 1 July 2019 for Rev.9. UR S6 “does not apply to CSR Bulk Carriers and Oil Tankers”. Those ships follow the same table in CSR Pt 1 Ch 3 Sec 1 Table 7.
UR S6 Table 1 places members in three categories:
- Secondary members (A1 to A3): Class I within 0.4L amidships, grade A or AH outside
- Primary members (B1 bottom plating including keel, B2 strength deck plating and others): Class II within 0.4L, grade A or AH outside
- Special members (C1 sheer strake, C2 stringer plate, and others): Class III within 0.4L, Class II outside 0.4L, Class I outside 0.6L
Single strakes of Class III are at least 800 + 5L mm wide, and need not exceed 1,800 mm “unless limited by the geometry of the ship’s design”. Plating materials for sternframes, rudders, rudder horns and shaft brackets are in general not below Class II. Rudder plates at stress concentrations are Class III. The sheer strake and stringer plate are the typical Class III members.
UR S6 Table 2 covers ships longer than 150 m with a single strength deck, excluding liquefied gas carriers covered in Table 3. It requires grade B or AH within 0.4L for the longitudinal members of the strength deck. Under CSR [2.3.2], members not in the CSR tables take grade A or AH “upon agreement of the Society”. CSR [2.3.3] keeps stern frames and shaft brackets at Class II or above.
Grade by thickness
UR S6 Table 7 gives the grade for each class and thickness band. UR S6.1 states: “The steel grade is to correspond to the as-built plate thickness and material class.” Figure 3 shows the table as a step chart.
| As-built thickness (mm) | Class I | Class II | Class III |
|---|---|---|---|
| t ≤ 15 | A/AH | A/AH | A/AH |
| 15 < t ≤ 20 | A/AH | A/AH | B/AH |
| 20 < t ≤ 25 | A/AH | B/AH | D/DH |
| 25 < t ≤ 30 | A/AH | D/DH | D/DH |
| 30 < t ≤ 35 | B/AH | D/DH | E/EH |
| 35 < t ≤ 40 | B/AH | D/DH | E/EH |
| 40 < t ≤ 50 | D/DH | E/EH | E/EH |
Reading the table
Two trends run through Table 7. In the mild steel column, a Class II plate moves from A to B above 20 mm. It moves to D above 25 mm and to E above 40 mm. At 22 mm the mild steel column gives A, B and D for Classes I, II and III. The higher tensile column gives AH, AH and DH.
The table has separate mild steel and higher tensile columns. Where mild steel takes B, the higher tensile column takes AH, because there is no BH grade. For D and E, the letters match. A Class III plate of 32 mm is E in mild steel and EH in higher tensile steel, so EH36 for 355 N/mm². The number of a grade comes from the strength check through k, and the letter from UR S6.
For ships over 250 m, UR S6 Table 4 requires the sheer strake and deck stringer plate in E or EH within 0.4L. The bilge strake takes D or DH. UR S6 Table 5 covers single-side skin bulk carriers subjected to SOLAS regulation XII/6.4. Their lower brackets and side shell strakes take D or DH. Table 6 covers ice strengthening, and S6.2 ships for low air temperatures, such as those under the Polar Code.
Worked example: the sheer strake
Take a sheer strake of 32 mm in AH36 within 0.4L of a ship of 200 m. These are example values.
- Find the category. The sheer strake is special member C1.
- Find the class within 0.4L. Class III.
- Find the grade at 32 mm. Table 7 gives E/EH for 30 to 35 mm.
- Name the steel. The 355 N/mm² steel in grade E is EH36.
The same plate outside 0.6L, in Class I, needs only B/AH, which for higher tensile steel is AH36.
YP47 steel and extremely thick plates in container ships
YP47 is steel of 460 N/mm² minimum yield for the upper deck region of large container ships, under IACS UR W31 and UR S33. UR W31 Rev.3 (March 2023), “YP47 Steels and Brittle Crack Arrest Steels”, covers YP47 for “longitudinal structural members in the upper deck region of container carriers”. The thickness is over 50 mm up to 100 mm.
UR W31 Table 2 gives grade EH47: thermo-mechanically controlled, yield 460 N/mm², tensile 570 to 720 N/mm². Its elongation is 17%, and it is impact tested at −40 °C. The Charpy energy is 53, 64 and 75 J for 50 to 70, 70 to 85 and 85 to 100 mm. UR W31 1.1.2 states: “Unless otherwise specified in this UR, UR W11 is to be followed.” Table 1 limits the EH47 chemistry to carbon 0.18% maximum and manganese 0.90 to 2.00%. Silicon is 0.55% maximum, and phosphorus and sulfur 0.020% each.
UR W31 was first issued in January 2013, with Rev.1 in September 2015, Rev.2 (a complete revision) in December 2019 and Rev.3 in March 2023. The original applied to ships contracted on or after 1 January 2014. Rev.3 applies to manufacturer approval applications dated on or after 1 July 2024.
UR S33 and the material factor of YP47
IACS UR S33 Rev.3 (February 2020), “Requirements for Use of Extremely Thick Steel Plates in Container Ships”, applies to YP36, YP40 or YP47 steel in the upper deck region. The thickness is over 50 mm up to 100 mm. Rev.3 applies to ships contracted on or after 1 July 2021. The upper deck region covers “upper deck plating, hatch side coaming plating, hatch coaming top plating and their attached longitudinals” (1.1.5).
UR S33 1.2.1 notes that YP36, YP40 and YP47 refer to minimum yield strengths of 355, 390 and 460 N/mm². Under 1.2.2, YP47 plate is to be EH47 to UR W31. Plates over 100 mm are left to the Society (1.3.2).
UR S33 1.4.1 states: “The material factor of YP47 steel for the assessment of hull girder strength is to be taken as k = 0.62.” That value is not in UR S4. Under UR S33 1.1.3, three measures apply in accordance with Annex 1, which sets them by yield strength and thickness. They are non-destructive testing in construction, periodic non-destructive testing after delivery, and brittle crack arrest design. Under 2.1.1, ultrasonic testing to UR W33 covers all block-to-block butt joints of the upper flange members in the cargo hold region. Under 4.1.1, the brittle crack arrest steel method is usable where the upper deck grade is not higher than YP40. Otherwise other means are agreed. Fatigue follows the Society’s rules (1.4.2).
The UR S33 stub records the UR separately.
Brittle crack arrest
UR W31 defines two brittle crack arrest grades. BCA1, for 50 to 100 mm, has a crack arrest toughness Kca at −10 °C of at least 6,000 N/mm^3/2. A crack arrest temperature of −10 °C or below also qualifies. BCA2, for 80 to 100 mm, has a Kca of at least 8,000 N/mm^3/2. UR W31 1.3.1 allows the brittle crack arrest designation on YP36 and YP40 steel under UR W11 as well as on YP47. The brittle fracture article covers the failure mode.
The MLIT final report of March 2015 records YP47 steel of 460 N/mm² in the hatch coaming of the 8,110 TEU MOL Comfort. The committee inferred that the “hull fracture originated from the bottom shell plates in the midship part”. The ultra large container ship and container ship articles cover the ship type.
Choosing between mild steel and higher tensile steel
The rules make higher tensile steel pay only where a yield-based limit governs the scantling. Each limit below comes from a rule named in this article:
| Limit | Effect of higher tensile steel | Rule |
|---|---|---|
| Hull girder section modulus | Falls with k | UR S11.3.1.1; CSR Pt 1 Ch 5 Sec 1 |
| Hull girder moment of inertia | Unchanged | UR S11.3.1.2; CSR IyR |
| Plating under lateral pressure | Falls roughly with √(235/ReH) | CSR Pt 1 Ch 6 Sec 4 [1.1.1] |
| Minimum thickness | Unchanged | CSR Pt 1 Ch 1 Sec 2 [5.2.1] |
| Corrosion addition | Unchanged | CSR Pt 1 Ch 3 Sec 3 [1.1.1] |
| Elastic buckling | Unchanged for the same thickness | UR S11.5; CSR Ch 8 |
| Welded joint fatigue | Not raised | UR W11 2.3 Note 1 |
| Toughness | Set by the grade letter, not the strength level | UR W11; UR S6 |
The table is a Shipping-Wiki.com construction. The flanges of the hull girder in a long ship, where the section modulus governs, gain most. Members at their minimum thickness, members governed by stiffness, and welded details governed by fatigue gain least.
The same rules apply to a bulk carrier, an oil tanker and a container ship. At the same displacement, less lightweight means more deadweight. The gas carrier cargo containment uses other materials, which the cryogenic materials article covers.
Applying higher tensile steel in a design
A designer who specifies higher tensile steel checks each limit that the steel changes and each limit it does not. The steps below follow the rules named in this article:
- Find the required section modulus with k, under UR S11 or CSR Pt 1 Ch 5 Sec 1.
- Choose the grade of each member from its UR S6 class and its as-built thickness.
- Check the vertical and longitudinal extent of the higher strength steel, under CSR Pt 1 Ch 5 Sec 1 [2.4].
- Check the plate slenderness and the buckling capacity of the thinner plating.
- For 390 N/mm² steel at k = 0.66, perform the fatigue assessment that UR S4 requires.
- Check the welded details in fatigue, because UR W11 2.3 Note 1 gives them no strength gain.
- Check the minimum moment of inertia, which has no k.
- Record the steel types and grades in the plan kept on board, under CSR [2.1.5].
For a container ship with plates over 50 mm in the upper deck region, add the UR S33 measures and the UR W31 steel. A finite element analysis of ship structures gives the local stresses at the hatch corners and the coaming ends, where the thick plates meet.
A grade choice made only for the section modulus can fail at step 4 or step 6, and the scantling then rises again. The CSR hull girder checks use the n50 section properties, with half the corrosion addition deducted. The local plating checks use the full net thickness.
Higher tensile steel in service
In service, a renewed plate takes the grade of the as-built plan, and the plan of steel types and grades is kept on board. CSR Pt 1 Ch 3 Sec 1 [2.1.5] requires that plan. The approved scantlings assume the as-built grade and strength level, so a renewal in a lower grade does not match the approved plan. The classification society holds the approved plans.
The continuous survey and the close-up survey of the Enhanced Survey Programme gauge the plating against the renewal criteria. IACS Rec 47 covers the repair quality standard, and non-destructive testing the weld inspection.
Revision dates of the steel URs
The steel URs apply by contract date or by the date of the manufacturer approval, so the revision in force depends on the ship. The table lists the revisions and their application as stated in each UR:
| UR | Current revision | Applies to |
|---|---|---|
| UR S4 | Rev.4, April 2017 | Non-CSR ships; k definition |
| UR S6 | Rev.9 Corr.2, November 2021 | Rev.9 from 1 July 2019 |
| UR W11 | Rev.9, May 2017 | Ships contracted on or after 1 July 2018 |
| UR W11 | Rev.10, September 2025 | Ships contracted on or after 1 January 2027 |
| UR W31 | Rev.3, March 2023 | Manufacturer approval applications from 1 July 2024 |
| UR S33 | Rev.3, February 2020 | Ships contracted on or after 1 July 2021 |
| UR W16 | Rev.3, March 2016 | Rev.4 from 1 January 2027; not hull steel |
The contract date follows IACS PR 29. The Unified Requirements reach the ship through the rules of each IACS member.
Common errors about hull steel and k
Several statements about higher tensile steel do not match the UR texts. Each line gives the statement, then what the rule says.
- “UR S4 gives k = 1.0 for mild steel.” UR S4 lists only 315, 355 and 390 N/mm² steel. The 1.0 is in UR S7.1 and CSR Table 2.
- “UR S4 sets how far higher tensile steel extends.” UR S4 has no extent rule. The CSR extent rule is Pt 1 Ch 5 Sec 1 [2.4].
- “The CSR allows k = 0.66 for 390 N/mm² steel.” The CSR gives 0.68 only. The 0.66 value, with a fatigue assessment, is in UR S4 for non-CSR ships.
- “UR S4 gives k = 0.62 for YP47.” The 0.62 value is in UR S33 1.4.1, for hull girder strength.
- “UR W16 is the YP47 rule for container ships.” UR W16 excludes commercial hull steel. YP47 is in UR W31, used with UR S33.
- “UR W11 has a 265 N/mm² strength level.” UR W11 has three higher strength levels, 315, 355 and 390 N/mm².
- “Higher tensile steel raises fatigue strength.” UR W11 2.3 Note 1 states the opposite for welded joints.
- “Higher tensile steel makes the hull stiffer.” E is the same for all carbon steel grades, and the minimum inertia carries no k.
Limitations
This article summarizes the IACS steel and strength URs and the CSR named in the sources. They include UR S4, S6, W11, W31 and S33, and the CSR of 1 July 2025. The class rules and the approved plans of a ship decide its steel.
- The worked examples and the ratios of Figure 2 are Shipping-Wiki.com arithmetic from the rule formulas, not values for a real ship.
- The plate thickness ratio √(235/ReH) applies to “other members” in the CSR formula. Longitudinal members take a different Ca.
- Weight savings from higher tensile steel depend on the design and are not stated in the rules summarized.
- The UR S6 low air temperature rules and the UR S33 Annex 1 measures by thickness are not detailed here.
- ASTM designations such as A36 are a different standard and are not compared here.
Frequently Asked Questions (FAQs)
What is higher tensile steel?
Higher tensile steel is hull structural steel with a specified minimum yield stress above the 235 N/mm² of normal strength steel.
The CSR calls it HT, against MS for mild steel, and IACS UR W11 covers the levels of 315, 355 and 390 N/mm².
What does AH36 mean?
AH36 is higher strength hull steel of 355 N/mm² minimum yield, grade A, impact tested at 0 °C.
The CSR writes AH36; IACS UR W11 writes A36 for the same steel.
What is the difference between AH36 and DH36?
Both have a minimum yield stress of 355 N/mm².
AH36 is impact tested at 0 °C and DH36 at −20 °C, under IACS UR W11, so DH36 has proven toughness at a lower temperature.
What do the grade letters A, B, D, E and F mean?
They give the Charpy impact test temperature.
For normal strength steel, A is +20 °C, B 0 °C, D −20 °C and E −40 °C. For higher strength steel, A is 0 °C, D −20 °C, E −40 °C and F −60 °C (UR W11 Rev.9).
What is the tensile strength of AH36?
UR W11 Rev.9 and CSR Pt 1 Ch 3 Sec 1 Table 1 give a tensile strength of 490 to 630 N/mm² for the 36 level, with a minimum yield of 355 N/mm².
What is the material factor k for 355 N/mm² steel?
0.72, under IACS UR S4 Rev.4 and CSR Pt 1 Ch 3 Sec 1 Table 2.
The factor is 0.78 for 315 N/mm² and 0.68 or 0.66 for 390 N/mm².
Why are there two k values for 390 N/mm² steel?
UR S4 allows k = 0.66 provided that a fatigue assessment of the structure is performed to the Society’s requirements, and 0.68 in other cases.
The CSR gives 0.68 only.
Does UR S4 give k = 1.0 for mild steel?
No. UR S4 lists only the higher tensile steels.
The value of 1.0 for ordinary hull structural steel comes from UR S7 and CSR Pt 1 Ch 3 Sec 1 Table 2.
Does UR S4 apply to CSR ships?
No. UR S4 states that it does not apply to CSR bulk carriers and oil tankers.
Those ships take k from CSR Pt 1 Ch 3 Sec 1 Table 2.
What k does the CSR give for steel above 390 N/mm²?
None.
CSR Pt 1 Ch 3 Sec 1 [2.2.1] leaves steel above 390 N/mm² to the Society on a case by case basis, and interpolates k linearly between the listed values.
What is the material factor of YP47 steel?
IACS UR S33 Rev.3 1.4.1 takes k = 0.62 for YP47 steel in the assessment of hull girder strength.
YP47 has a minimum yield of 460 N/mm².
Where is YP47 steel used?
IACS UR W31 Rev.3 covers YP47 for longitudinal structural members in the upper deck region of container carriers, at thicknesses over 50 mm up to 100 mm.
What is brittle crack arrest steel?
Steel proven to stop a running brittle crack.
UR W31 defines BCA1 for 50 to 100 mm with a crack arrest toughness Kca at −10 °C of at least 6,000 N/mm^3/2, and BCA2 for 80 to 100 mm with at least 8,000.
When does UR S33 apply?
To container ships with YP36, YP40 or YP47 steel over 50 mm and up to 100 mm thick in the upper deck region.
Rev.3 applies to ships contracted on or after 1 July 2021.
Does higher tensile steel raise fatigue strength?
Not for welded joints.
IACS UR W11 Rev.9 2.3 Note 1 states that the effective fatigue strength of a welded joint of higher strength steel ‘may not be greater’ than in normal strength steel.
Does higher tensile steel make the hull stiffer?
No. CSR Pt 1 Ch 3 Sec 1 [2.1.1] takes E as 206,000 N/mm² for all carbon steel.
The CSR minimum moment of inertia and the UR S11.3.1.2 minimum carry no k, so they do not fall with higher tensile steel.
Does buckling strength rise with yield stress?
Only partly. The elastic buckling stress depends on E and the plate slenderness, not on the yield.
The yield enters the critical stress only above half the yield, through the Johnson-Ostenfeld correction of UR S11.5.
How does plate thickness change with yield stress?
Under lateral pressure, CSR Pt 1 Ch 6 Sec 4 [1.1.1] gives a net plate thickness proportional to 1/√ReH for other members, so higher tensile plating needs less net thickness.
AH36 plating is therefore about 0.81 of the mild steel thickness.
Do minimum thicknesses fall with higher tensile steel?
No.
CSR Pt 1 Ch 1 Sec 2 [5.2.1] states that the minimum thickness is independent of the specified minimum yield stress.
Does the corrosion addition change with steel grade?
No.
CSR Pt 1 Ch 3 Sec 3 [1.1.1] applies the corrosion additions to carbon-manganese steels with no distinction by strength.
How far must higher strength steel extend vertically?
CSR Pt 1 Ch 5 Sec 1 [2.4.1] sets the vertical extent zhts,i of at least z1 (1 − σperm,i/σL), from the deck or the bottom.
Below that extent the stress is within the permissible value of the lower steel.
What are the UR S6 material classes?
UR S6 places each member in Class I, II or III by its category (secondary, primary or special) and position.
Special members such as the sheer strake and stringer plate are Class III within 0.4L amidships.
What grade does a 32 mm Class III plate need?
Grade E, or EH for higher tensile steel, under UR S6 Table 7 and CSR Pt 1 Ch 3 Sec 1 Table 7.
What changes for ships longer than 250 m?
UR S6 Table 4 requires the sheer strake and stringer plate at the strength deck in grade E or EH, and the bilge strake in D or DH, within 0.4L amidships.
What is new in UR W11 Rev.10?
UR W11 Rev.10 (September 2025) applies to ships contracted on or after 1 January 2027.
The strength levels and the tensile values are unchanged, and clause 1.5 covers the optional approval for high heat input welding.
Does UR W16 cover hull steel?
No. UR W16 states that it does not apply to steels for the hull structure of commercial ships, whose requirements are in UR W11.
UR W16 covers high strength steels of 420 to 960 N/mm² for welded structures.
Can an owner limit the use of higher tensile steel?
Yes, as an owner’s extra.
CSR Pt 1 Ch 1 Sec 2 [3.10.1] lists a maximum percentage of high strength steel among the owner’s extras.
What steel record must be kept on board?
CSR Pt 1 Ch 3 Sec 1 [2.1.5] requires a plan of the steel types and grades used in the hull to be kept on board.
Which grade replaces a renewed plate?
The grade of the as-built plan.
UR S6 states that the steel grade corresponds to the as-built plate thickness, and the plan of steel types and grades records it.
Did higher tensile steel play a part in the MOL Comfort loss?
The MLIT report of March 2015 records YP47 steel of 460 N/mm² in the hatch coaming of MOL Comfort.
The committee inferred that the hull fracture originated from the bottom shell plates in the midship part.
No question matches. Try a shorter or different word.
Sources
- IACS UR S4 Rev.4 (April 2017). Criteria for the Use of High Tensile Steel with Minimum Yield Stress of 315, 355 and 390 N/mm2 iacs.s3.af-south-1.amazonaws.com
- IACS UR S6 Rev.9 Corr.2 (November 2021). Use of Steel Grades for Various Hull Members, Ships of 90 m in Length and Above iacs.s3.af-south-1.amazonaws.com
- IACS UR W11 Rev.9 (May 2017). Normal and Higher Strength Hull Structural Steels iacs.s3.af-south-1.amazonaws.com
- IACS UR W11 Rev.10 (September 2025). Normal and Higher Strength Hull Structural Steels iacs.s3.af-south-1.amazonaws.com
- IACS UR W31 Rev.3 (March 2023). YP47 Steels and Brittle Crack Arrest Steels iacs.s3.af-south-1.amazonaws.com
- IACS UR S33 Rev.3 (February 2020). Requirements for Use of Extremely Thick Steel Plates in Container Ships iacs.s3.af-south-1.amazonaws.com
- IACS UR W16 Rev.3 (March 2016). High Strength Steels for Welded Structures iacs.s3.af-south-1.amazonaws.com
- IACS CSR BC&OT (1 January 2024 with 1 July 2025 Corrigenda). Common Structural Rules for Bulk Carriers and Oil Tankers iacs.s3.af-south-1.amazonaws.com
- IACS UR S11 Rev.10 (Dec 2020). Longitudinal Strength Standard iacs.s3.af-south-1.amazonaws.com
- IACS UR W16 Rev.4 (September 2025, Corr.1 March 2026). High Strength Steels for Welded Structures iacs.s3.af-south-1.amazonaws.com
- MLIT Committee on Large Container Ship Safety. Final Report (English version), March 2015 mlit.go.jp
- IACS UR S7 Rev.4 (May 2010). Minimum Longitudinal Strength Standards iacs.s3.af-south-1.amazonaws.com